Three projects on what it takes for a mineral residue to become a usable construction material.
VANDERSANDEN · HORIZON EUROPE
Carbon4Minerals
Work Package 4 leader · Vandersanden
Can steelmaking residues become a reliable raw material for a brick manufacturer?
The Lanklaar pilot brings semi-dry pressing and CO₂ curing into an operating factory. Slag is blended with other constituents and pressed into shape. During curing, CO₂ reacts with minerals in the slag to form carbonates that bind the brick together.
I lead Work Package 4. My work at Vandersanden covers formulation, troubleshooting and pilot implementation for facing bricks and pavers. The wider Horizon Europe consortium connects CO₂ capture, mineral processing and product demonstration across eight planned industrial pilots.
Up to 80%Steelmaking by-products in the facing bricks described by the Lanklaar pilot team
2,000 tonnesPublished pilot production target for facing products using ArcelorMittal slags
VITO’s primary research fellow on BnB · Postdoctoral appointment
Can old concrete supply both the aggregate and part of the binder for new concrete?
BnB brought Belgian and Dutch partners together to separate demolished concrete into usable fractions. My work at VITO examined two routes, carbonating the recovered aggregate and thermally reactivating the hardened cement paste. I was first author on the studies of both routes.
In our aggregate experiments, moisture before curing made a decisive difference. The air-dried material absorbed 3.82% water after carbonation, down from 5.26% for untreated aggregate. Under the same carbonation conditions, aggregate that started wet absorbed 5.45%.
Water absorption of recycled coarse aggregateMeasured after treatment, % by mass
Untreated control5.26%
Wet before carbonation5.45%
Air-dried before carbonation3.82%
The two treated samples were carbonated for 4 hours at 20 °C and 5 bar CO₂, without added water vapour. Selected observations from Table 5, experiments 1, 7 and 15.
The binder study exposed a different trade-off. More intense heat treatment increased the measured reactivity of recovered paste. Yet among the treatments we tested, 350 °C for two hours gave the best overall strength performance in the blends.
VITO’s primary research fellow on SlagVal · Postdoctoral appointment
After recovering valuable metals, can the remaining slag replace some of the cement in mortar?
SlagVal linked metal recovery to the use of the remaining mineral fraction. At VITO, I investigated three treated non-ferrous metallurgical slags as supplementary cementitious materials and was first author of the resulting publication.
We replaced 30% of the cement by mass in the test mortars and examined strength development and leaching. All three treated slags showed limited reactivity. The crushed mortars met the heavy-metal leaching limits used in the study. For a producer, those findings answer two questions about how much the slag contributes to strength and how the material behaves at end of life.